Grade C35E 1.1181

» Materials » EN Specifications » Grade C35E 1.1181

This European Standard specifies requirements for semi-finished products, bars and rods for fasteners with properties specified at elevated and/or low temperatures made of non-alloy and alloy (including stainless) steels and nickel alloys as given in Table 1. The requirements of this standard may be applied also to the finished fasteners. The general technical delivery conditions in EN 10021 also apply to products supplied in accordance with this European Standard.


Chemical Composition

Material designation Chemical composition, % by mass
Element Number C Si Mn P max. S max. Altot B Cr Mo Ni V Others
C35E 1.1181 0,32 to 0,39 ≤ 0,40 0,50 to 0,80 0,030 0,015 b ≤ 0,40 ≤ 0,10 ≤ 0,40 Cr+Mo+Ni: ≤ 0,63

Mechanical Properties

Material designation Heat treatment condition a Diameter c (d mm) Proof strength (Rp0,2 MPa min.) Tensile strength (Rm MPa) Elongation after fracture (A % min) Reduction in area (Z % min) Impact energy (ISO-V) at 20 °C (KV2 J min)
Name Number
C35E 1.1181 +N d ≤ 60 300 500 to 650 20 27
+QT d ≤ 60 340 560 to 710 22 45 55
60 < d ≤ 150 340 560 to 710 22 45 39